Tnt Chain Bend Old No. Unks Anl1ude Pre- Breaking Percent Broken Between Remarks
No. sample angle ratio of In angle stress load alrelght link IInb
links contact load (Ib) 8trength
(Ib)

23 B go. 2.3 8 2 -go. 130,000 - - - - Chain first pre·
3 Flat slressed to 130,000
o· - - - - - 154.300 98 .6% 8" 7-8 Ib 10 cause signifi·
cant chain deforma·
lion. Test chain lhen
8\raight break tesled

24 A O· - (^6) - - - 173.600 >93% Shackle - Straight break lest
o. unbroken section
01 chain from lesl
1 0 including
severely deformed
links. Broke in
shackle before
chain broke



  • InrlicaJes bl'6ilk OCC!j!1lld In straight chatn link Whlch was nol m conlact wllh curved sul1tJGe.


TABLE F.2: (continued)

1.0


  • J:


t;

Z w

~ 0.8

" Z Si:
~

~


0

-^0


./


I
lE: -
m
I-J:

"


06
~
I-
~ J:

.. FI~tChatn
f-
I-
"

o SecOl1d Chain
Z W
lE: 0.4
l-(/)
eI
z
:2 f-
~
a:
m 0.2
::E
::J
::E
~
::E

f-

0 I I I t I I I I I I I I
o 5 10 IS

SURFACE TO CHAIN DIAMETER RATIO Old

FIGURE F9: RESU1.. TS OF TESTS OF CHAIN TENSIONED OVER CURVED SURFACE