Steels_ Metallurgy and Applications, Third Edition

(singke) #1

Table 43(a) (continued)


Chemical composition (cast dysis)') offemtic stainless steek

Steel designation %bymaSS


Name Number C Si Mn P S N Cr Mo Nb Ni zi Others
marmarmarmar mar

X2CrMoTi 18-2 1.4521 0.025 1.00 1.00 0.040 10.015 0.030 17.00 to 1.80 to 4x (C+N)


X2CrMoTiS18-2 1.4523 0.030 1.00 0.50 0.040 0.15 to 17.50 to 2.00 to 0.30 to (C + N)
0.35 19.00 2.50 0.80 5 0.040
X6CrNi 17- 1 1.4017 0.08 1.00 1.00 0.040 10.015 16.00 to 1.20 to
18.00 1.60
X6CrMoNb 17- 1 1.4526 0.08 1.00 1.00 0.040 10.015 0.040 16.00 to 0.80 to 7 x (C+N)
18.00 1.40 M.10 to 1.00
X2CrNbZrl7 1.4590 0.030 1.00 1.00 0.040 10.015 16.00 to 0.35 to zr27X
17.50 0.55 (C + N)


X2CrAlTil8-2 1.4605 0.030 1.00 1.00 0.040 10.015 17.00 to 4x (C+N) Al: 1.70
18.00 fo.15 to O.8d) to 2.10
X2CfliNbl8 1.4509 0.030 1.00 1.00 0.040 10.015 17.50 to 3 x C+0.30 0.10 to 0.60
18.50 to 1.00
X2CrMoTi29-4 1.4592 0.025 1.00 1.00 0.030 10.010 0.045 28.00 to 3.50 to 4x (C+N)
30.00 4.50 +0.15 to 0.8d)


20.00 2.50 +0.15 to 0.8d)


+0.15

')Elements not listed in this table may not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast. All appropriate
precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production which would impair mechanical properties and
the suitability of the steel.
')For bars, rods, sections and the relevant semi-finished products, a maximum content of 0.030% S applies.
For any product to be machined, a controlled sulphur content of 0.015% to 0.030% is recommended and permitted.
3)The stabilization may be made by use of titanium or niobium or Zirconium. According to the atomic number of these elements and the content of carbon and
nitrogen, the equivalence shall be the following:


*Patented steel grade.