Steels_ Metallurgy and Applications, Third Edition

(singke) #1

Table 43b) (continued)


Chemical composition (cast analysis)'' of manemitic and precipitation hardening stainless steels

Steel designation %bymaSS


Nm Number dL) Si Mn P S Cr cu Mo Nb Ni others
mM.max.mar
~ ~~
XWrMoV 18 1.4112 0.85 to 1.00 1.00 0.040 10.0153) 17.00 to 0.90 to V: 0.07 to
0.95 19.00 1.30 0.12


0.22 17.00 2.50

14.00 0.70 4.50

17.00 1 SO 6.00

17.00 5.00 to 0.45 5.00

18.00 7.80") 1.50

16.00 3.00 7.80 1.50

15.00 2.00 2.00 0.60 6.00

X17CrNi 16-2 1.4057 0.12 to 1.00 1.50 0.040 10.0153) 15.00 to 1.50 to


XSCrNiMo 13-4 1.4313 10.05 0.70 1.50 0.040 50.015 12.00 to 0.30 to 3.50 to N: I 0.020


X4CrNiMol6-5- 1 1.4418 50.06 0.70 1.50 0.040 ~0.015~) 15.00 to 0.80 to 4.00 to N 2 0.020


xSCrNiCuNbl6-4 1.4542 10.07 0.70 1.50 0.040 10.0153) 15.00 to 3.00 to 50.60 5 x C 3.00 to


X7CrNiAll7-7 1.4568 10.09 0.70 1.00 0.040 10.015 16.00 to 6.50 to Al: 0.70 to


X8CrNiMoAl15-7-2 1.4532 50.10 0.70 1.20 0.040 10.015 14.00 to 2.00 to 6.50 to Ak 0.70 to


xSCrNiMduNbl4-5 1.4594 10.07 0.70 1.00 0.040 10.015 13.00 to 1.20 to 1.20 to 0.15 to 5.00 to


')Elements not quoted in this table may not be intentionally added to the steel without the agreement of the purchaser except for 6nishing the cast. AU appropriate
precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production which would impair mechanical properties and
the suitability of the steel.
2)Tighter carbon ranges may be agreed at the time of enquiry and order.
3)F0r bars, rods, sections and the relevant semi-finished products, a maximum content of 0.030% S applies. For any product to be machined, a controlled sulphur
content of 0.015% to 0.030% is recommended and permitted.
4)F0r better cold deformability. the upper limit may be increased to 8.30%.

Free download pdf