344 Steels: Metallurgy and Applications
100
A
o
2 50
r
p-^2
f
f
G~
I,,. I I I
0 0.5 1.0 1.5
Log o -~
Figure 4.27 True stress-true strain in 18% Ni base steels with different chromium levels
(After Llewellyn and Murray 2s)
140
120
04 .-.^100
r-
N 80
e-
,-. 60
.~ 4o
e- |
~ 20
301
201
347
r~o2
(^304 321
10
0
80
o~
,- 60
.g
t..-^40
_o
uJ
2O
-- 1" 301
J 302
304
,~ } 321
316
-347 ~."~~,~=
310~
0 10 20 30 40 50 60 70 80
Reduction (%)
Figure 4.28 Effect of coM rolling on the tensile strength and elongation of austenitic
stainless steels (After Llewellyn and Murray 2s)