GTBL042-14 GTBL042-Callister-v2 August 29, 2007 8:59
582 • Chapter 14 / Synthesis, Fabrication, and Processing of Materials
8620
(0.2 wt% C)
8630
(0.3 wt% C)
8640
(0.4 wt% C)
8660
(0.6 wt% C)
Hardness, HRC
20
40
50
60
170 70 31 18 9 5.6 3.9 2.8 2
490 305
270
125 56 33 16.3 10
Cooling rate at 700°C (1300°F)
7 5.1 3.5
°C/s
°F/s
30
Distance from quenched end
0 10 20 30 40 50 mm
0 14 12 34 1 14 12 111 34 2 in.
Figure 14.9
Hardenability curves for
four 8600 series alloys of
indicated carbon content.
(Adapted from figure
furnished courtesy
Republic Steel
Corporation.)
Hardness, HRC
20
40
50
60
170 70 31 18 9 5.6 3.9 2.8 2
305 125 56 33 16.3 10
Cooling rate at 700°C (1300°F)
7 5.1 3.5
°C/s
°F/s
30
Distance from quenched end
10 20 30 40 50 mm
490
270
0
0
1
4
1
2
3
4 1
1
4
1
2
111 3
4 2 in.
Figure 14.10 The
hardenability band for an
8640 steel indicating
maximum and minimum
limits. (Adapted from figure
furnished courtesy
Republic Steel
Corporation.)