Scintillation Detectors 83
T
able
8.1. Characteristics of different solid scintillation detectors.*
Effective atomic
Density
Scintillation
Photon yield
Linear atten. coeff
Energy resolution
Detectors
no (Z)
(g/cm
3 )
decay time (ns)
(per keV)
(cm
−^1 ) of 511 keV
(% at 511 keV)
NaI(Tl)
51
3.67
250
38
0.34
†
10
BGO
74
7.13
300
6
0.92
20
BaF
2
54
4.89
0.6
2
0.44
11.4
GSO
59
6.71
60
10
0.70
8.5
Anthracene
—
—
26
30
—
—
LSO
66
7.40
40
29
0.87
10
YSO
34
4.53
70
46
0.39
12.5
CsI(Tl)
‡
54
4.51
1000
52
0.48
§
—
* BGO, bismuth germanate; BaF
, barium fluoride; LSO, lutetium oxyorthosilicate; YSO, yttrium oxyorthosilicate; GSO, gadolinium oxyorthosilicate. 2
†
The linear attenuation coefficient of 140 keV photons of
99m
Tc in NaI(Tl) is 0.155 cm
−^1.
‡
Early P, Private communication, 2005.
§
Of 660 keV.