Scanning Electron Microscopy and X-Ray Microanalysis

(coco) #1

387 23


Analysis with a compromised sample shape:
surface gouge crater left by tool impact
a

Mg (normalized weight percent)

Fe (normalized weight percent)

Analysis of K411: Bulk polished and tool gouge crater

0

5

10

15

20

25

30

35

40

012345678910 11 12

BULK-K411

BULK-600grit

1

Extent of ideal
flat specimen
measurements

b

. Fig. 23.8 a SEM (ET+)
SE + BSE image of a crater pro-
duced in polished K411 glass
after gouging with a diamond
scribe. b Plot of the normalized
Mg and Fe concentrations calcu-
lated for measurements at vari-
ous locations in this crater